Toksan technical blog · Turning

If your insert lasts only 20 parts on a 42CrMo4 shaft, chip control is often the issue

In the workshop, problems turning 42CrMo4 are often blamed on the insert. If the edge discolours after 15–25 parts on a quenched and tempered shaft, first check whether the chips are breaking.

Toksan technical team · 30 August 2026 · 11 min read
Turning 42CrMo4 with a ZCC-CT CNMG rhombic insert in its holder
Negative ZCC-CT rhombic insert (CNMG) in its holder. This is the standard shape used here for 42CrMo4. Source: ZCC Cutting Tools Europe.

Turning 42CrMo4 is often dismissed as a “bad insert”. On a quenched and tempered shaft, the edge turns brown-blue after 15–25 parts. A new box may add only ten parts. If YBC is the indicated grade, inspect chip breaking before switching grades.

What you will learn

  • 42CrMo4 (1.7225 / AISI 4140) concentrates heat at the edge. If the chip does not curl, friction can cause the CVD coating to flake.
  • The PM chipbreaker needs a depth of cut of 1.5–3 mm. A supposedly safe cut of 1.2 mm does not break the chip, even with the same grade.
  • Standard stock setup: CNMG120408-PM + YBC252 (ZCC-CT, CVD, ISO P20–P35). Tighten the screw with a torque wrench.
  • Inspect the edge after ten parts. Adhesion, crater wear and the fracture of a single corner point to different causes.

Why 42CrMo4 and C45 behave differently in turning

42CrMo4 is a chromium-molybdenum steel for quenching and tempering (EN 1.7225, AISI 4140), distinct from C45. Applications include automotive shafts, pins, gear bodies and tractor components. Toksan’s ISO P steel range lists 4140 (42CrMo4), 4340, C45 and 16MnCr5. Sharing a stock category does not make these steels interchangeable.

Do not confuse the material conditions. Annealed or normalised shafts produce relatively soft chips. A quenched and tempered (+QT) shaft at 28–34 HRC tends to produce sticky chips, retain heat at the edge and cause abrasive wear from chromium carbides. Hardened surfaces above 50 HRC call for CBN or ceramic rather than simply slowing a YBC grade.

42CrMoS4 behaves differently. Sulphur shortens chips and improves tapping and turning. With 42CrMo4 without the S addition, stringy chips are more likely. Check the material certificate before changing the insert.

With a stable machine, carbide cutting speeds are roughly 220–300 m/min (Machining Doctor gives 225–305 m/min for turning 4140). This is a range, not a fixed setting of Vc 280. If feed f and depth of cut ap fall outside the chipbreaker’s range, the edge rubs at 280 m/min.

Turning 42CrMo4: why poor chip breaking can lead to coating flaking

42CrMo4 retains heat at the edge. If the chip does not curl and break, it rubs against the coating. The YBC family’s TiCN + Al₂O₃ CVD layer can then flake, leaving the edge apparently worn out after 15–25 parts.

Changing the grade code does not stop this mechanism. If chips remain stringy, changing from YBC252 to YBC351 may only buy another ten parts. How to select a cutting insert also applies here: material, operation, chipbreaker, then grade. Swapping one YBC grade on the shelf for another skips the diagnosis.

ZCC-CT YBC CVD-coated rhombic insert: chipbreaker pockets, 08 nose-radius code (0.8 mm) and 42CrMo4 turning
ZCC-CT YBC, CVD-coated 80° rhombic insert with visible chipbreaker pockets. If the chip does not enter the pocket, it rubs against the coating. Source: Toksan / ZCC-CT.

Studies of tool wear and chip breaking in AISI 4140 report a similar effect. As the tool wears when turning 42CrMo4, chipbreaker performance and chip control deteriorate. The relationship can also run the other way: long chips can contribute to premature edge failure.

PM chipbreaker range: a supposedly safe 1.2 mm depth of cut may leave the chip unbroken.

ZCC-CT PM chipbreaker is designed for medium machining to roughing. Its approximate range is ap 1.5–3.5 mm and f 0.22–0.35. Reducing ap to 1.0–1.4 mm to protect the edge can keep the chip from entering the chipbreaker. Long, stringy chips wrap around the edge and strip the coating. Check the operating range before blaming the chipbreaker.

A misleadingly “safe” setting PM range (medium machining) FM (finishing)
ap 1.0–1.4 mm 1.5–3.5 mm 0.3–1.0 mm
f 0.16–0.20 mm/rev 0.25–0.32 mm/rev 0.10–0.18 mm/rev
Chipbreaker PM (outside the operating range) PM FM
Chips Stringy chips wrap around the edge Short, curled C- or 6-shaped chips Thin, controlled chips
Cutting edge after 20 parts Discolouration and flaking Even flank wear Finishing marks

Change one thing at a time. Either bring ap into the PM range at 2.5–3 mm or switch to FM or a narrower chipbreaker. Keep the grade unchanged. In many workshops this adjustment alone doubles tool life in 42CrMo4 turning.

The GH chipbreaker is for heavier roughing and requires a higher feed. Without interrupted facing cuts or cast pockets, PM is sufficient. Taking a 0.4 mm finishing pass with PM makes the same mistake at the other end of the range.

Coolant hose present, but the jet misses the cutting zone

If the coolant misses the cutting zone, the edge turns brown-blue. An open hose alone does not establish effective cooling. A jet missing the cutting point can result in a vapour layer, heat build-up at the edge and increasing crater wear.

With through-coolant delivery, check the pressure. A weak jet fails to clear chips from the pocket and chips can strike the edge. Align the coolant jet with the cutting point and then verify pressure. For a brown edge, check the jet direction before the grade.

ZCC-CT zRay through-coolant delivery: jet directed at the cutting zone when turning 42CrMo4
The jet is aimed at the cutting point. A hose pointing behind the workpiece does not provide the same cooling. Source: ZCC-CT zRay, Toksan archive.

When turning 42CrMo4, high-pressure coolant through the bar or holder pushes the chip against the chipbreaker. External flooding can leave chips on the part. A high-pressure turning holder such as ZCC-CT zRay directs the jet where it helps clear the chip and relieve the edge.

High cutting speed and low feed cause rubbing at the edge

Vc 280 with f 0.18 may look like a precision setting. In 42CrMo4 the low feed can take the cut below minimum chip thickness. The edge rubs instead of cutting, heats up, changes colour and can be worn out after 20 parts.

Keep the grade and set f to 0.28–0.32. If the finish deteriorates, try a wiper insert before reducing the feed again. In many 42CrMo4 operations, feed is the main influence on Ra. Lowering the speed can make the edge rub without improving the finish. Cutting range: starting values for steel, cast iron and stainless steel.

Inspect the chip before changing the grade. If the chip does not break, YBC252 is unlikely to be the cause.

Stock tooling for turning 42CrMo4: CNMG120408-PM YBC252

ZCC-CT turning tools: holders for CNMG rhombic inserts, stock tooling for 42CrMo4
ZCC-CT turning tools. Standard tooling for 42CrMo4: CNMG120408-PM + YBC252 in a C-shaped seat. Source: ZCC Cutting Tools Europe.

ZCC-CT describes YBC252 as a CVD-coated P20–P35 grade for medium machining through roughing of steel and cast steel, balancing wear resistance and toughness. This is also the designation on Toksan’s ISO P stock: CNMG120408-PM YBC252 — 80° rhombic insert for medium machining to roughing.

For dimensions, designations and options, consult the CNMG insert size and selection guide for more details.

How to read the code:

  • C — 80° rhombic insert for straight diameters and facing. For profile shoulders, use DNMG (55°) in its own seat.
  • N — 0° clearance, negative, double-sided, 4 corners.
  • M — medium tolerance.
  • G — cylindrical hole, chipbreakers on both sides.
  • 12 — 12.7 mm edge (IC).
  • 04 — 4.76 mm thick.
  • 08 — 0.8 mm nose radius. Use 04 for finishing, 12 for roughing.
  • PM — chipbreaker for medium machining.
  • YBC252 — grade for steel.

Within this family, use YBC151 for continuous finishing (higher wear resistance, thinner edge) or YBC351 for interrupted roughing (P20–P40, toughness for low-speed roughing). Stay with 252 when turning a straight 42CrMo4 shaft in a continuous cut. Switch to 351 if the corner breaks, but not for stringy chips alone.

Incorrect screw tightening can damage the seat and cause vibration attributed to a “bad insert”. Use a torque wrench. A DNMG insert does not belong in a C-shaped seat. The holder and insert shape designations must match. Technical pages: General turning catalogue (PDF), grade overview ZCC-CT Europe grade overview.

Inspect the cutting edge after ten parts

Toksan test and demonstration centre: turning trial on 42CrMo4 with an EMCO Hyperturn
EMCO Hyperturn at the Toksan test and demonstration centre. During the 42CrMo4 trial, the edge is inspected after 10 parts. Source: Toksan.
What does the edge look like? Cause First corrective action
Brown-blue discolouration Heat: chips are not breaking or the coolant jet is missing Bring ap into the PM range and aim the hose at the cutting zone
Built-up edge (BUE) Low f, low Vc, blunt edge set f to 0.28. For further details, see in the article on built-up edge (BUE) — the same mechanism occurs less often in 42CrMo4
Crater wear (depression on the rake face) High Vc, no coolant, friction from chips Set Vc to 220–240 and measure through-coolant pressure
Chipping at one corner Torque, insert seat, toolholder, impact in interrupted cuts Check the clamping first. Use YBC351 for interrupted cuts.
Long, stringy chips Depth of cut outside the chipbreaker’s range ap 2.5–3 mm or FM
Even flank wear Normal tool life Reduce Vc slightly or switch to 151 for finishing

Inspect after 10 parts rather than waiting for 200. Look for short C-shaped chips in the bin, not stringers. Photograph the edge, chips and insert label, and record Vc, f and ap. This helps identify whether the chipbreaker, coolant delivery or clamping torque needs attention.

Example: Ø60 quenched-and-tempered shaft, continuous external turning

Workpiece: 42CrMo4 +QT, approximately 30 HRC, Ø60, length 180 mm. Continuous external turning, roughing and finishing. Machine: 15 kW, hydraulic chuck and tailstock centre. Toolholder with a C-shaped insert pocket.

Roughing Finishing
Insert CNMG120408-PM YBC252 Same insert seat, FM or wiper 08
Vc 240–260 m/min 260–280 m/min
f 0.28 mm/rev 0.18–0.22 (0.28 with a wiper insert)
ap 2.5 mm 0.4–0.6 mm
Chips Short C- or 6-shaped chips Thin, broken chips

An unsuitable combination for the same shaft is a PM chipbreaker, ap 1.2 mm, f 0.16 and Vc 280. The chips become stringy and the edge turns blue after 20 parts. Switching to YBC351 does not correct these conditions. Bring ap and f into the working range.

For interrupted roughing across keyseats or keyways, consider YBC351 while keeping the PM operating range. For thin walls or long overhang, first L/D and clamping — a wiper and high feed cannot mask vibration.

Frequently asked questions

Which insert is the starting point for turning 42CrMo4?

CNMG120408-PM with YBC252. Use a torque wrench and keep ap within the PM chipbreaker range. For finishing, use YBC151 with FM geometry or a wiper. Use YBC351 for interrupted roughing. For stainless steel, switch to YBG to avoid adhesion on YBC.

Should I switch grades if the insert lasts only 20 parts?

No. First inspect the chips, coolant jet and feed range. Change the grade last.

When should I use FM instead of PM?

At ap below 1 mm, the PM chipbreaker is outside its working range. Switch to FM or increase ap to 2.5 mm. Change one setting at a time.

Is Vc 280 too high when turning 42CrMo4?

Not on its own. In combination with f 0.18, rubbing can occur. Raise f to 0.28–0.32. If discolouration persists, lower Vc to 220–240.

Do 42CrMo4 and 42CrMoS4 use the same insert?

Use the same grade family. The sulphur-bearing version produces shorter chips, but the chipbreaker range still depends on ap. Look for the S in the material certificate.

Where can I obtain a genuine ZCC-CT insert for 42CrMo4?

Toksan has been an authorised ZCC-CT distributor in Türkiye since 2004. Send us your holder code, hardness (HRC) and cutting conditions (Vc/f/ap). Contact.

Availability and application support

Send Vc, f, ap and a photo of the part

For 42CrMo4 turning, we assess the chipbreaker, coolant delivery and clamping torque and respond the same day.

Quotes and technical support Turning insert